A Peel Strength Tester measures the force needed to separate bonded materials while a specimen is peeled at a specified angle and rate. When the method calls for a mean force normalised by specimen width, the peel strength formula is mean peel force divided by measured specimen width. Use force in newtons and width in millimetres to get N/mm. Multiply by 25 to express the same result in N/25 mm if your report calls for that unit.
The calculation is the same at 90° and 180° when both methods call for the same width-based quantity. The test arrangements and measured forces can differ. At 90°, the free strip pulls approximately perpendicular to the bonded surface at the peel front. At 180°, the strip folds back over the still-bonded length. The method also determines which part of the force record to evaluate and whether to report a mean, a peak or additional observations. The examples below illustrate the arithmetic, with no prescribed specimen dimensions, rates or acceptance values.
What does a Peel Strength Tester measure?
The load cell records how much force the grip applies as the bond separates. A controlled drive moves the grip or fixture while the arrangement maintains the required peel geometry. The peel front is the boundary between material that has separated and material that remains bonded. It advances during the test. For a repeatable result, control what happens at that front as well as what the crosshead displays.
The result describes a bonded construction in its test condition. The adhesive, the surface underneath it and the flexible layer that bends as it is peeled all contribute to the response. A shipping label, pressure-sensitive tape, bonded laminate and flexible package seal may all be examined using a force machine, but each must follow the appropriate method. For a broader introduction to films and laminates, see Pacorr's guide to mechanical testing of films and laminates.
How do 90° and 180° peel setups differ?
Use the direction along the bonded strip toward the peel front as the reference for the angle of pull on the free arm. At 90°, the peeled strip leaves the front approximately at right angles to the bonded surface. A suitable moving table or equivalent fixture can keep the front aligned with the pulling direction as the test progresses. At 180°, the free strip folds back over itself and pulls approximately parallel to the substrate. The drawing shows common geometries. The exact grip and fixture arrangement comes from the method.
| Feature | 90° peel | 180° peel |
|---|---|---|
| Free arm at the peel front | Pulled away from the plane of the bonded surface. | Folded back over the bonded length. |
| Fixture focus | Track the moving front so the prescribed angle is maintained. | Keep the fold-back path aligned and free from unintended contact. |
| Result identity | Record 90° with the method, rate, width and force statistic. | Record 180° with the method, rate, width and force statistic. |
A specimen that is set at 90° at the start can move out of angle as the front travels. Check the geometry over the measured interval. At 180°, a backing that curls, creases or tears in the fold can change how the specimen responds. Document unusual deformation or contact and apply the method's test validity rules.
How do you calculate peel strength from measured force?
For a method using mean-force normalisation, write P = F̄ ÷ b. F̄ is the mean valid peel force over the specified analysis interval in N. The symbol b denotes the measured specimen width in mm, taken across the strip perpendicular to its length. The resulting P is in N/mm. Use the applicable method's width definition, measurement positions and rounding rule. Preserve the original trace and specimen dimensions for an independent check.
Peel length specifies how far the separation progresses or the portion of a record to analyse. It does not enter the width denominator. Width also differs from thickness. Normalising by width gives a force-per-width result. Multiplying width by thickness and dividing force by area would address a different property, such as a stress in a tensile test performed with a suitable method.
How do N, N/mm and N/25 mm differ?
A force channel reports N. A peel strength expressed per width has a width basis attached to the force. The notation N/25 mm gives a result referred to a 25 mm width. A narrower measured strip can be expressed in that unit when the method permits. Preserve the measured width so the report never suggests that an arithmetic normalisation was a test of a different physical specimen.
| Result or reference unit | Calculation for a width-based mean result |
|---|---|
| N | Mean force from the specified trace interval. Report this separately if required. |
| N/mm | Divide the mean force in N by measured width in mm. |
| N/25 mm | Multiply the numerical N/mm value by 25. Divide by 25 to go back to N/mm. |
| N/cm | Multiply the numerical N/mm value by 10. |
For example, 0.300 N/mm can be written as 7.50 N/25 mm or 3.00 N/cm. A result reported as N/25 mm differs from a reading of 7.50 N unless the raw trace and width establish that force. If a method specifies a particular unit or specimen width, give it priority over the expression most convenient for your worksheet.
How do you calculate peel strength for a 90° test?
Suppose a fictional 90° specimen gives a mean force of 6.0 N over the valid interval and has a measured width of 20.0 mm. Divide 6.0 by 20.0 to obtain 0.300 N/mm. Multiply by 25 for 7.50 N/25 mm. The displayed digits show the arithmetic. Use the method's precision when reporting a real specimen.
This example uses one mean force after evaluating the correct part of the trace. If a software field holds the tallest point or an average of the entire travel, importing it into the formula will produce a different result. Check the trace interval and the statistic selected during instrument setup before reviewing any result in N/mm.
How do you calculate peel strength for a 180° test?
Suppose a separate fictional 180° specimen gives a mean force of 9.6 N and has a measured width of 24.0 mm. Calculate 9.6 ÷ 24.0 = 0.400 N/mm, equivalent to 10.0 N/25 mm. The two example specimens have different inputs and illustrate their own calculations. They do not represent the same material tested at both angles or specify standard specimen widths.
If the 180° example were entered with a default width of 25 mm, the worksheet would give 0.384 N/mm. That is 4% below the value calculated from the 24.0 mm entered above. Check the actual measured width and keep the raw force with the reported result. Measure and normalise each valid specimen separately before forming an average if the method calls for specimen-based results. Ratios from varying widths can differ from a ratio calculated using group mean force and group mean width.
How do you read a peel force trace?
A peel trace plots force against elapsed time, crosshead travel or measured distance peeled, depending on the test system. The start can include slack take-up, a force rise or an initial peak. The running part may be relatively smooth or may show repeated peaks as peeling advances. Release or tearing can change the trace near the end. Retain the complete curve and use the interval and statistic specified by the method.
When the method uses distance peeled, confirm how that distance is measured or derived. Crosshead travel can include the movement of a fixture and length changes in the specimen. It is not automatically the same as advance of the peel front. If the data are unevenly spaced along the relevant distance, a simple mean of displayed samples can over-represent the densely sampled segments. Follow the prescribed evaluation or software procedure instead of assuming a particular averaging rule fits every export.
Should you use the initial peak, maximum or mean peel force?
Use the statistic named in the method or purchase specification. A start-up peak can describe initiation while the specified running mean describes propagation. If both are required, label their windows and units separately. For example, ASTM D1876 determines T-peel resistance over a specified length after the initial peak. ASTM F88/F88M identifies maximum seal force as important and also discusses average force for some applications. Those choices belong to the respective methods. ASTM D1876 and ASTM F88/F88M.
Agree the analysis settings before evaluating lots. Keep the same rule for how a run starts, ends and qualifies for an average. If a spike appears inside a relevant window, inspect the specimen and grip history. Follow the method for including the force event, documenting an abnormal failure or repeating an invalid test. Discarding inconvenient force values makes results difficult to reproduce.
Can you convert a 90° result to a 180° result?
There is no universal conversion factor between 90° and 180° peel results. The angle changes how the backing bends and how force is applied at the peel front. Material stiffness, stretch, adhesive response, thickness, peel speed and failure mode can all influence the measured resistance. A switch from N/mm to N/25 mm changes the unit expression of one valid result. A change of angle requires its own measurement for a comparison.
When a customer requests a method change, agree which specimens, surface preparation, ageing and conditioning will be used, then run both methods on representative material. Carry individual results and failure observations into the review. A relationship developed for one construction and set of conditions cannot automatically transfer to another tape, backing or substrate.
Which peel standard fits your specimen?
Start with the specimen type and property named by the purchase specification or development programme. Identify the controlled edition, geometry, adherends, test conditions and reporting requirement. That decision comes before fixture selection or unit conversion.
| Standard or method | Relevant scope |
|---|---|
| ASTM D3330/D3330M-04(2025) | Pressure-sensitive tape. Method A is a 180° measurement and Method F a 90° measurement for single-coated tape on the specified surface. |
| ISO 29862:2024 | Self-adhesive tapes. Methods 1–4 cover different 180° peel adhesion measurements. |
| ASTM D6862-11(2021) | Adhesive bond joining a flexible adherend to a rigid adherend, approximately 90°. |
| ASTM D903-98(2025) | Comparative peel or stripping characteristics of adhesive bonds under defined conditions. Uses approximately 180° in its stripping procedure. |
| ISO 8510-2:2006 | 180° peel resistance of a bonded assembly with one flexible and one rigid adherend. |
Method A and Method F of ASTM D3330/D3330M specify a standard steel panel or other surface of interest for single-coated tape. The series has separate methods for other tape or liner arrangements. Under ISO 29862, the four listed 180° methods address peel from stainless steel, peel from the tape's own backing, double-sided and transfer tapes, and liner adhesion. Use the applicable method number in a report. ASTM D3330/D3330M and ISO 29862:2024.
ISO lists ISO 8510-1:1990 as withdrawn and ISO 8510-2:2006 as current. If an existing contract cites the withdrawn 90° reference, confirm the controlled method with the customer before switching. ASTM D6862 is a current option for an appropriate flexible-to-rigid 90° adhesive assembly where the requirement permits it. ASTM D6862, ASTM D903, ISO 8510-2 and ISO 8510-1 status.
How do T-peel and flexible seal strength fit in?
In a T-peel test, two flexible adherends separate and their free ends are pulled in opposing grips. The T-peel specimen has a different geometry from a flexible strip peeled back against a rigid supporting panel. ASTM D1876 addresses relative peel resistance in the T-type specimen. ASTM F88/F88M measures a strip containing a seal in flexible barrier materials and records failure mode. Follow its applicable tail support arrangement and force reporting rather than borrowing a tape peel acceptance value.
Seal-strip results describe the sampled seal and its test configuration. If a laminate splits or the film tears instead of the seal separating, the force is tied to that observed failure. A strip test also cannot answer every question about leaks or opening an entire package. See Pacorr's guide to distinguishing seal failure from film failure.
How do you prepare tape or bonded specimens?
Identify the material and surface under test. Cut straight strips in the direction required and check width at the prescribed places. Track backing direction, substrate lot and adhesive face when relevant. Use the specified panel material and surface preparation. Residual adhesive, dust, surface treatment and handling marks can change what happens at the interface. Follow the approved cleaning procedure and avoid touching a prepared bond surface.
Use the prescribed application or bonding method, including the specified pressure or roller conditions for pressure-sensitive tape where applicable. For a bonded assembly, retain relevant cure and adhesive preparation records. Allow the required dwell between application and peel, and condition specimens according to the method. Pressure-sensitive contact can develop during dwell, while heat, moisture and cure affect other adhesive systems. A fixed sequence helps make runs comparable without assuming that one laboratory's conditions apply to all materials.
What is a practical peel test procedure?
Use this educational workflow to plan the test. Let the applicable method, material specification and instrument instructions set the exact dimensions, environment, speed, fixtures, preparation, operating precautions and validity rules.
- Confirm the standard, edition, angle and property required. Record the specimen construction and substrate condition.
- Prepare and identify the strips. Measure widths and follow the required application, cure, dwell or conditioning procedure.
- Fit the required fixture, grips and force measurement range. Verify zero, alignment, angle, motion, speed and available travel under the method.
- Mount the panel or lower assembly and grip the free strip centrally. Check the free path, initial position and any preload or tare specified by your procedure.
- Run the specified motion and record the force curve. Observe grip movement, peel front alignment, tearing or changes in failure behaviour.
- Evaluate the method-defined window and statistic. Apply width normalisation where required and retain the individual results and failure observations.
- Review repeats, deviations and group summaries. Clean contact parts as specified and preserve the original data with the report.
A machine can perform repeatable motion even when the angle or sample preparation is wrong. For a new setup, review a representative trial curve and the physical peeled specimen before standardising the programme. Pacorr's Peel Strength Tester setup overview.
Why do peel rate, dwell and conditioning matter?
An adhesive can respond differently when separation is fast, slow, warm or cold. Backing deformation and the way the peel front advances can also depend on speed. The target value may refer to crosshead speed or to rate of separation under the method. Check the definition and fixture kinematics rather than transferring a number between machines without context.
Keep the application sequence and dwell history with the force trace. A strip peeled soon after applying it may respond differently after a longer dwell. Similarly, a cured or aged joint can need a condition-specific plan. If two labs use nominally similar tests but disagree, compare temperatures, humidity where relevant, application or cure history, surface preparation and rate before treating the difference as supplier variation.
What do the common peel failure modes mean?
Interfacial failure occurs at a boundary between adhesive and adherend. Cohesive failure occurs within the adhesive layer, and material may remain on both surfaces. A backing or substrate tear occurs within an adherend, while a laminate may split between constituent layers. A sample can show more than one mode along its length. Keep the peeled faces and identify where each observation occurred.
A specimen that tears through its backing can show that the applied force caused a material failure before a clean adhesive peel was observed in that configuration. Preserve the actual failure and apply the governing method to reporting and interpretation. A specimen that slips in a grip instead raises a test validity question. Use the accepted terminology and any requested proportions or photographic evidence. ISO 10365:2022 failure-pattern designations.
What causes unexpected peel results?
Begin with the original trace, photos and preparation notes. Compare the conditions before attributing a shift to the adhesive. Median or mean values can hide a change from interfacial peeling to material failure across replicates. Review specimen-level results and apply the documented acceptance or investigation rule.
| Observation | Useful first check |
|---|---|
| One edge leads the peel front. | Check grip alignment, cut squareness and whether the fixture permits the intended motion. |
| Force rises while the panel moves or the arm touches hardware. | Inspect fixture freedom, clearance and angle across the measured interval. |
| Result changes after a software export update. | Compare raw force units, width entry, selected analysis interval and requested statistic. |
| Force changes between panels or operators. | Review panel identity, substrate preparation, pressure, dwell and conditioning. |
If the values vary within a roll, map the strip locations and orientation. If they vary by instrument, circulate matched specimens under one agreed method and inspect both fixtures before pooling data. Track changes in material, operator and fixture separately when planning the investigation.
What belongs in a peel strength report?
A result needs its geometry, unit and relevant test condition. In the arithmetic example, the 90° mean was 6.0 N on a 20.0 mm strip, giving 7.50 N/25 mm. The accompanying record identifies how the average was obtained. Keep the unit and rate in the same record as the number to avoid ambiguity during incoming inspection or a customer audit.
| Report field | What to keep |
|---|---|
| Specimen and method | Material, lot, adherends, side and direction, standard edition and method, peel angle and measured width. |
| Preparation and condition | Substrate treatment, application, dwell or cure, and relevant conditioning and environment. |
| Machine and analysis | Fixture, load range and units, verified speed, analysis interval and force statistic. |
| Results and disposition | Original force curve, width-based value with unit, failure mode, valid count, summary and governing decision rule. |
Distinguish results for individual specimens from the summary. Keep standard deviations or other statistics where required. A specific material or purchase limit can apply to an individual minimum, a group mean, a peak or a combination. Use the rule agreed for the product and record exclusions and authorised repeats.
How do you verify the tester and choose a useful force range?
Select a load cell and measurement range suited to the expected low and high peel loads. A maximum capacity or a fine display increment tells only part of the story. Ask for evidence of force verification over the actual working interval. Check zero, speed and displacement as required. Verify that the fixture maintains its intended geometry during travel and that the grip retains the strip without cutting or slipping.
Maintain grips and guides so that wear, adhesive residue and fixture friction are detected. Use the approved cleaning and verification procedures. Document changes after moving, repairing or replacing a fixture or load cell. If a display label is ambiguous, confirm its unit against the manufacturer and force verification record before converting. For confirmed kilogram-force readings, 1 kgf = 9.80665 N. NIST force conversion factors.
What does Pacorr publish for the PCPSTD-1?
Pacorr's Peel Strength Tester listing identifies the tabletop PCPSTD-1. The page and linked brochure list a 20 kgf load capacity, 500 mm maximum grip-to-grip distance, an S-type load cell and a digital load display. They show a 40–400 mm/min drive range and a separate 300 mm/min test-speed entry. The published default jaws are vise type. Check the usable travel, precise speed and required fixture for the specific method. The maximum distance between grips does not establish usable test travel for every configuration.
The catalogue uses kg-style display wording. Confirm the actual output unit and force range of the supplied configuration. If your method requires an analysis window, saved curves, downloadable data or automatic average calculation, verify those functions in the quoted configuration. The public listing describes displayed load values. Ask whether the 90° and 180° fixtures and any required motion arrangement are included for your specimen.
What affects the price of a Peel Strength Tester?
Price depends on the force range, included angle fixtures, jaw type, usable travel, curve recording, software export and verification documentation. Service, training and installation may also affect delivered cost. Pacorr's listing describes a general price range across configurations. Request a written quote for the exact model and accessories required by your test.
Include the specimen construction and width, expected force, required angle, standard, speed, failure observations and reporting format. Demonstrating the specified hardware and analysis with your sample gives more relevant evidence than relying only on a catalogue list of compatible standards.
Frequently asked questions
What is the peel strength formula?
For a method requiring width-normalised mean force, divide the mean force in newtons over the prescribed analysis interval by measured strip width in millimetres. The result is in N/mm.
How do I convert N/mm to N/25 mm?
Multiply the numerical N/mm value by 25. For example, 0.300 N/mm equals 7.50 N/25 mm. Retain the actual tested width and use the output unit required by the method.
Is the formula the same at 90° and 180°?
The same width normalisation applies when both methods use that result definition. The angle, fixture and specimen response can change the mean force and the resulting peel strength.
Can one 90° value be converted to a 180° result?
There is no universal conversion. Test the required geometry under the governing method, or use a controlled comparison to study the relationship for a specific construction.
Should I use the maximum force or the average force?
Use the method's defined statistic and portion of the trace. A start or maximum force and a running mean describe different parts of the test and should be identified separately where both are required.
What width should I use in the calculation?
Measure across the actual strip at the locations required by the method. Keep the tested width in the record even when the result is normalised to a reference width such as 25 mm.
Which ASTM tape method uses 90° peel?
For single-coated pressure-sensitive tape on the specified panel or surface, ASTM D3330/D3330M Method F is the 90° method. Method A measures the corresponding 180° arrangement.
What if the film tears before the adhesive peels?
Record the tear and where it occurred. The force reflects the observed specimen response, so the reporting and validity rules come from the applicable method.
Is a peel strength value the same as tensile stress?
Peel strength under a width-normalised method is force per width. Tensile stress is force per cross-sectional area. Use the property definition and units given in the test specification.
How can Pacorr help configure your peel test?
Send your specimen construction, required method and edition, peel angle, measured widths, typical force range and output needs. Include any 90° tracking fixture, 180° arrangement, specialised grips or curve export your test requires. Contact Pacorr to discuss the configuration and request a quotation.