Izod and Charpy impact tests measure how a specimen responds to a sudden pendulum strike. In a common notched Izod setup, a vise clamps the specimen vertically and the striker hits above the notch from the notched side. In a common notched Charpy setup, the specimen lies horizontally on two supports and the striker hits near the middle from the face opposite the notch. Both methods start with an energy measurement in joules. The standard tells you whether to report those joules, divide by specimen width, or divide by a cross-sectional area.
For a width-based plastics result, impact resistance in J/m = 1,000 × corrected energy in J ÷ specimen width in mm. For a notched area-based plastics result, impact strength in kJ/m² = 1,000 × corrected energy in J ÷ remaining area in mm². A metallic Charpy test typically reports absorbed energy in J. Use the method as well as the unit to identify each result. The examples below explain the arithmetic and the decisions needed for a repeatable lab comparison.
What is the difference between Izod and Charpy impact testing?
Izod loads a cantilever. Its fixture fixes one end while the free portion bends under impact. Charpy loads a bar on two supports. The striker loads the span between the supports. That change in how the specimen bends can change its failure mode and measured energy. When the test is specified as notched, the notch concentrates stress at a controlled position.
| Feature | Common notched Izod | Common notched Charpy |
|---|---|---|
| Specimen fixture | Upright in a vise with one end held. | Horizontal on two supports. |
| Striker face | Usually approaches the notched face. | Approaches the face opposite the notch. |
| Strike position | Above the notch and clamped region. | Near midspan, opposite the notch. |
| Record to compare | Method, configuration, energy and the specified reporting unit. | Method, configuration, energy and the specified reporting unit. |
The diagram illustrates conventional arrangements. A specified reversed-notch Izod method, an unnotched option or a different blow direction calls for its own setup. Follow the drawing in the selected standard for strike position, notch alignment and fixture geometry. For the machine components and an overview of operation, see Pacorr's IZOD and Charpy equipment guide.
What does the pendulum actually measure?
The pendulum begins with gravitational potential energy at its release position. It accelerates as it falls, strikes the specimen and rises with the energy remaining after impact. In a simple model, the indicated energy loss is m × g × (h₁ − h₂). Here m is the swinging assembly mass, g is gravitational acceleration and the two heights are measured for its centre of mass from a common datum. The instrument normally uses its verified energy scale or angle measurement to give the corresponding energy indication.
The nominal capacity of a hammer is its available energy for the configured setup. The test reading is the energy removed from the swing during that particular test, with method-specified corrections. Part of the loss can come from machine friction, air resistance and the indicating mechanism. Specimen deformation and fracture can also take different shares of the measured energy. Applying a pendulum energy formula to a display value alone cannot separate these contributions. NIST reference on Charpy absorbed energy.
When do you subtract a friction or windage correction?
Follow the test standard and the machine's instructions for verifying the empty swing and applying the prescribed correction. Some scales or digital modes already compensate for the machine's losses. Record what the instrument reports before transferring the result to a worksheet. A second subtraction from a compensated reading introduces a systematic error. Some methods call for other adjustments in defined circumstances, so avoid treating one empty-swing number as a universal correction for every hammer and release configuration.
For arithmetic only, a raw loss of 2.08 J minus a valid correction of 0.08 J gives 2.00 J. A display already confirmed to show 2.00 J corrected enters the calculation directly. A drifting empty-swing check warrants investigation before a test. The energy used to throw broken specimen pieces is another contribution. ASTM D6110 describes this contribution without establishing a correction procedure for it. Keep any correction from a different method out of the Charpy calculation.
How do you calculate an ASTM width-based result in J/m?
The denominator in a width-based result is the measured specimen width specified by the method. For the conventional milled-notched configurations discussed here, this is the dimension parallel to the notch line, across the specimen from one end of that line to the other. The remaining depth from the notch root to the opposite face describes a different dimension. Verify the drawing before entering values, especially when software labels the first dimension as thickness instead. ASTM D6110 uses a width-based result. ASTM D256 covers width-based and, where applicable, area-based reporting, so read the required form in the material specification and procedure. ASTM D256 and ASTM D6110.
For a fictional width-based record, let the corrected energy be 2.00 J and the measured width be 10.00 mm, or 0.01000 m. Calculate 2.00 ÷ 0.01000 = 200 J/m. Dividing by 10.00 gives 0.200 J/mm, the same ratio expressed per millimetre. Apply the factor of 1,000 when the inputs are joules and millimetres and the required output is J/m. These values show the calculation. Use the controlled method for acceptable specimen dimensions.
How do you calculate an ISO area-based result in kJ/m²?
For a notched plastic specimen, the ligament is the material left at the cross-section between the notch root and the opposite face. In the rectangular example here, its area equals specimen thickness multiplied by the remaining width. Measure both quantities as the method requires. For an unnotched area-based configuration, use the full cross-sectional area specified by the method. Using the original width in a notched calculation includes the material removed by the notch and makes the reported value too low.
In a separate illustrative record, the specimen thickness is 4.00 mm, its remaining width is 8.00 mm and corrected absorbed energy is 2.00 J. The remaining area is 32.00 mm². Calculate 1,000 × 2.00 ÷ 32.00 = 62.5 kJ/m². One square millimetre is 0.000001 m², while 1 kJ is 1,000 J. Together those conversions give the factor of 1,000. Retain the measured dimensions and raw energy values, then apply the specified rounding to the calculated result. ISO 180:2023 and ISO 179-1:2026.
What units belong on the test report?
The same display can show a raw energy channel and a calculated result. Give every column a property name and unit. A value of 200 can describe a width-based ratio or a raw energy, and those quantities answer different questions. Identify the method with its edition, option and specimen configuration next to the value.
| Reported quantity | Formula using joules and millimetres | Common reporting unit |
|---|---|---|
| Absorbed energy | Corrected energy from the method. | J |
| Width-based plastics impact resistance | 1,000 × energy ÷ measured width. | J/m |
| Area-based plastics impact strength | 1,000 × energy ÷ method-defined area in mm². | kJ/m² |
If a supplier uses a legitimate alternative unit for the same method-defined property, convert the unit while preserving the original result. For example, 62.5 kJ/m² equals 62,500 J/m². Unit conversions retain the quantity. Changing from length normalisation to area normalisation changes which quantity your report represents.
Can you convert Izod to Charpy or J/m to kJ/m²?
There is no universal Izod-to-Charpy conversion factor. Fixture geometry, specimen dimensions, notch shape, loading orientation and break behaviour can all change the energy term. A result from one method therefore cannot be reconstructed from the other merely by changing its denominator. To change a contract method, obtain agreement and test representative specimens in both configurations.
For the same valid raw record, a calculation can demonstrate the relationship between two normalisations when both are appropriate and the geometry is known. Suppose width is 10.00 mm and the dimension perpendicular to it remaining behind the notch is 8.00 mm. If the width-based result is 200 J/m, division by 8.00 mm gives a numerical value of 25.0 kJ/m² for that same record. The equality follows from the millimetre and kilojoule conversions. This example preserves the original measured energy, so it cannot predict the 62.5 kJ/m² in the separate ISO example with different dimensions.
How are metallic Charpy results different?
A metallic Charpy V-notch or U-notch method generally reports absorbed energy in joules. A measured value of 85 J remains 85 J on the energy line. The report also identifies the test temperature, specimen geometry and orientation. When using the ISO method for V-notch specimens, retain the applicable striker identification, such as the KV2 or KV8 designation for the configured striker radius. Record additional requested properties, such as lateral expansion or shear fracture appearance, under their own names and units.
Temperature can shift the response of some steels from more ductile to more brittle. A test programme may collect several valid results at each temperature to study the transition. A single value gives information about that specimen and condition. Report subsize specimens explicitly and follow the governing specification for interpretation. Multiplying or dividing by area alone cannot establish equivalence to full-size bars. ASTM E23-25 and ISO 148-1:2016.
Which impact test standard should your lab select?
Start with the material and the property required by your customer, product drawing or test programme. Record the standard edition specified in the contract. If it predates the latest published edition, clarify which applies before testing. Similar method titles can hide differences in specimen geometry, strike conditions and reporting.
| Standard | Scope and choice |
|---|---|
| ASTM D256-26 | Izod pendulum impact resistance of plastics. Select the required option and result expression. |
| ASTM D6110-26 | Charpy impact resistance of milled-notched plastic specimens. Reports energy per specimen width. |
| ISO 180:2023 | Izod impact strength of plastics within defined specimen and notch configurations. |
| ISO 179-1:2026 | Non-instrumented Charpy impact strength of plastics. Select the prescribed configuration and blow direction. |
| ASTM E23-25 | Notched-bar impact testing of metals, covering Charpy and Izod arrangements. |
| ISO 148-1:2016 | Non-instrumented V-notch and U-notch metallic Charpy energy testing. |
Treat a thin film, an entire part and a machined bar as different specimen systems. For film research, Pacorr's ASTM D1709 dart impact guide explains a falling-dart failure mass test. A tensile test answers questions about response under extension. Compare the specimen requirements in Pacorr's ASTM D638 and D882 guide when planning a broader plastics test programme.
How do notch radius, depth and material direction affect the result?
A sharper notch can concentrate stress more strongly and change where fracture starts. Notch depth affects the remaining section and can also change the specimen's fracture behaviour. Worn tools, burrs, heat from cutting and unintended gouges can introduce systematic differences across a batch. Inspect the notch against the specified profile with the nominated gauge or measuring system. Keep the notch tooling and inspection records with the job.
A moulded specimen and one cut from a sheet may carry different flow, reinforcement or residual-stress patterns. Identify extraction direction and the notch orientation relative to the material. Fibre-filled plastics, laminates and extruded sheet can give different values in different directions. Keep those directions separate in the report. For a notched versus unnotched investigation, test both only under their applicable configurations and draw comparisons within the designed study.
Why do temperature and conditioning matter?
Temperature, exposure time and moisture condition can affect the result, especially near a transition or for moisture-sensitive polymers. A new supplier's result at one condition and your incoming check at another may disagree even when both labs use the same standard name. Record the specimen preparation date where relevant, the conditioning history, the test temperature and any transfer requirements specified by the method. Use handling that preserves the required condition between removal and impact.
To investigate an unexplained shift, compare retained specimens under matched conditions, then vary one condition at a time. Separate differences caused by the material from differences introduced by a fixture, operator or data export. If a result belongs to an approved environmental study, keep each temperature and conditioning group independently recognisable in the data set.
What is a practical Izod or Charpy test procedure?
Use this educational sequence to plan a test. The selected standard, material specification, laboratory procedure and manufacturer instructions determine the exact geometry, settings, safety checks and validity criteria.
- Define the standard, edition, test option and result unit. Identify the lot, material direction, preparation route and conditioning plan.
- Prepare suitable specimens. Verify dimensions, notch profile, notch location and the measurement points named by the method. Retain individual readings for the denominator.
- Fit the prescribed fixture, striker and pendulum. Check that the verified working range and impact configuration suit the expected specimen energy. Perform method-required zero, loss and verification checks.
- Position each specimen against the relevant clamp or support datums. Check strike location and notch orientation. Follow the machine instructions for guards, release and recovery.
- Record the energy, correction state, specimen ID and break observation after each valid strike. Enter the individual width or area when the method calls for a normalised result.
- Review out-of-range indications and unusual fractures under the method's validity rules. Keep the raw record, authorised repeats, relevant failure categories and method-specific summaries.
Check a recorded result by independently calculating it from the raw energy and dimensions before relying on a new export mode. Verify that the selected scale, unit and specimen measurements match the worksheet. The screen can give a stable value even when its calculation mode is configured for a different test.
How do you choose a pendulum range?
Estimate the actual energy in joules expected from specimens. If the proposed width-based result is 200 J/m and measured width is 0.010 m, the implied absorbed energy is 2.0 J. For an area-based result, convert the units consistently and multiply by the expected area. Choose a verified hammer and range that meet the method's allowed fraction of available energy, impact speed and striker requirements across the expected workload.
A high capacity gives room for tougher specimens but can make a small energy loss harder to resolve. A too-light pendulum may leave the specimen unbroken or return a reading outside the method's usable range. A higher capacity by itself cannot fix alignment, fixture, notch or calibration errors. Where uncertainty is material to acceptance, ask for verification evidence at the actual range and configuration you will use.
How do complete, hinge, partial and non-break results differ?
Inspect each specimen and apply the method's failure categories. ASTM D256 distinguishes complete break, hinge break, partial break and non-break. It treats a non-break as a departure and groups averages by failure category when applicable. ASTM D6110 requires complete breakage for a standard result. Carry the specimen observations into the report and apply the counts, percentages and valid-result rules for your own method.
For example, eight complete breaks and two non-breaks warrant two observations in a lab review. The numerical result for the valid group describes that group's response. The other two observations show that some specimens behaved differently or need investigation under the governing rules. Recording just a mixed average discards that distinction. When the sample response changes unexpectedly, check repeatability, specimen geometry and pendulum range alongside the fracture appearance.
Which errors can distort an impact comparison?
First inspect the raw measurements and setup. Review the source of the corrected energy, actual orientation and measured dimensions before retyping a calculated result. A small error in the remaining section can change both the calculation and the physical test. For example, substituting 10.00 mm for an actual remaining width of 8.00 mm with 4.00 mm thickness and 2.00 J gives 50.0 kJ/m² instead of 62.5 kJ/m². That is a 20% understatement for the example.
| Observation | Practical check |
|---|---|
| All values shift after changing test mode. | Match the output unit, correction state, saved specimen dimensions and selected range. |
| Only one loading or material direction differs. | Confirm notch direction, strike face and specimen extraction markings. |
| Replicates vary after changing the notch cutter. | Inspect root profile, remaining section and preparation records. |
| Unexpected marks appear on the fixture. | Inspect striker alignment, support seating, specimen position and clearance under the method. |
Striker and support wear can change the contact geometry over time. Confirm the cause before combining results taken before and after adjustment. Where a failed verification affects released data, use your quality system to identify the affected period and disposition the results.
What should you record on an impact test report?
Retain readings per specimen and enough information for another lab to reproduce the comparison. A report line might read 62.5 kJ/m² for an illustrative area-based plastics calculation. The accompanying record should identify the method, specimen and fixture configuration, original energy, method-defined section and break category. The 62.5 value alone does not identify those conditions.
| Record item | What to capture |
|---|---|
| Method and specimen | Standard edition, option, specimen and lot ID, dimensions, notch and direction. |
| Test conditions | Conditioning history, temperature and departures. |
| Machine configuration | Instrument ID, striker, pendulum range, fixture and verification status. |
| Results | Energy, correction state, reported property with unit, break category, valid count and specified statistical summary. |
| Disposition | Applicable limits, acceptance rule and documented exclusions or repeats. |
Specify whether an acceptance requirement applies to each specimen, a valid group mean or a minimum value at a prescribed temperature. Keep report precision consistent with the method. For comparisons over time, note when an approved revision changed the specimen, fixture or calculation so the difference remains traceable.
What should maintenance and verification cover?
Keep fixture contact surfaces clean. Inspect the vise, anvils, striker, machine anchoring, pivot, zero indication and stopping or recovery systems using the instrument's approved maintenance instructions. Verify after installation, movement or repair when required and at the scheduled interval. Check the scope of calibration or verification evidence against the actual configuration. A generic certificate can omit the range or geometry being used.
For a plastics method, ISO 13802:2025 covers verification of relevant pendulum-machine properties. Applicable metallic Charpy programmes can include physical checks and indirect verification with certified reference specimens. Select the reference specimen level and striker configuration required by the governing method. NIST Charpy Machine Verification Program.
When do you need an instrumented impact test?
A non-instrumented pendulum records an overall energy change. An instrumented setup measures a force history with a suitable striker and measuring system. The selected method can use force versus displacement to study maximum force and energy associated with defined portions of the event. Digital energy readout alone does not establish that a machine supplies a verified force-time or force-displacement trace.
Ask for the acquisition channels, permissible speeds, data export and force verification if the requirement refers to a curve or a specific fracture event. ISO 179-2:2020 addresses instrumented Charpy impact testing for plastics. ISO 14556:2023 addresses instrumented Charpy V-notch testing for metallic materials.
What does Pacorr publish for the PCICIT-1?
Pacorr's IZOD / Charpy Impact Tester product listing identifies model PCICIT-1 with a listed 0–25 J impact energy range and a nominal 150° pendulum release angle. It describes separate hammers for Izod and Charpy, an Izod vise and a Charpy specimen support. The listing also describes a digital indication of energy and calculated outputs. Confirm the supplied hammers, scales, striker geometry, fixture dimensions and software result modes in the quotation.
An illustrative 85 J metallic Charpy result exceeds the published 25 J upper figure for this listing. It explains metal reporting only. A metallic specification requires a separate check of capacity, impact velocity, geometry and machine verification. Ask for the exact tested configuration and evidence for your required standard and edition before specifying a single frame for both material families.
What affects the price of an Izod or Charpy impact tester?
Pacorr provides a quotation route for the featured model. The delivered cost depends on the required energy ranges, included hammers and fixtures, compatible notching equipment, specimen measuring tools, verification or calibration documentation and optional data acquisition. Installation, operator training, freight and service coverage can also affect the quote. Send a specimen drawing or representative samples so the configuration discussion starts with the actual test.
Compare quotations for the same method and range. List the material, expected absorbed energy, notch configuration and working temperature. Ask which fixtures and verification records come with the machine. The listing gives general market guidance. Request a written quotation for the specific PCICIT-1 configuration.
Frequently asked questions
What is the main difference between Izod and Charpy?
Common Izod testing clamps one end of a specimen upright. Common Charpy testing supports a horizontal specimen at both ends and strikes near midspan. Follow the selected method for notch orientation and fixture dimensions.
What is the formula for a width-based impact result?
Multiply corrected absorbed energy in joules by 1,000 and divide by the method-defined specimen width in millimetres to get J/m.
How is notched impact strength calculated in kJ/m²?
Multiply corrected energy in joules by 1,000 and divide by the remaining cross-sectional area at the notch in square millimetres. Use the applicable area-based method.
Can I compare Izod with Charpy after converting units?
Only a unit conversion for the same method-defined property preserves the original measurement. Separate Izod and Charpy tests can give different energies, so a direct conversion cannot establish an equivalent result.
Why might a Charpy report show J instead of kJ/m²?
Conventional metallic Charpy methods report absorbed energy in joules. Area-based plastics methods instead normalise energy using a method-defined cross-sectional area.
Should I use the full section for a notched ISO plastics calculation?
Use the remaining area at the notch for the applicable notched calculation. The method's unnotched configuration defines the area to use for an unnotched test.
Should I subtract friction from a compensated display value?
If the displayed energy already includes the prescribed loss correction for the selected setup, use that corrected value. Check the instrument instructions and procedure before applying another correction.
What does a non-break mean on an ASTM D256 test?
It is a recorded failure category and a departure from the standard numerical result. Preserve the observation and follow the method's rules for reporting and calculating valid group summaries.
Does a digital tester always provide an instrumented impact curve?
An instrumented test needs suitable force measurement and acquisition. A digital energy display can report a pendulum reading without collecting a force-time or force-displacement curve.
How can Pacorr help configure your impact test?
Send your material, method and edition, specimen drawing, expected range in joules and the unit you need on reports. Include the pendulum configurations, notching, temperature control, verification evidence and data export your lab requires. Contact Pacorr to discuss the test and request a quotation.